ANH2

Cured Properties

Curing Properties

Composition:

  • 100 pbw digylcidyl ether of bisphenol A (Epon 828)
  • 80 pbw methyl-hexahydrophthalic anhydride
  • 30 pbw ARCOL 1025 polyol
  • 4 pbw 2-ethyl-4-methylimidazole
  • cured 4 hrs at 23C, 2 hr ramp to 60C, 6 hrs at 60C, 1 hr ramp to 93C, 12 hrs at 93C